Bending a LM tool
-
@BePrepared said:
Rebelgium, I got some spare can openers from LMs. I can give you one for testing. PM me an address. All I ask is for you to post some pics here of a red-hot LM can opener blade! (As long as it's safe to take pics while heating it up!)so, now asking for hot pics as payment huh
you should be ashamed on a public forum!!

-
OK, OK, I'd settle for some finished 'well dressed' pics. :-[
Drop me a PM, Rebelgium, and I'll send you a can opener.
-
-
-
-
-
-

Really cool stuff there! :o -
Nice work [emoji3]
[It's not failure if you learn something from it]
-
Yessss - nice one Zoidberg!!!

-
Nice work, and nice pics. I really like the way the tin-can was decimated. -
Nicely done Zoidberg

I Was really interested in the results
-
@Mechanickal I'm from Brugge
@bePrepared thanks a lot! PM sent
@Zoidberg wicked! Thanks for the experiments, very interesting!
So let me recap to see if I got this correctly:Cold bending with hammer snapped the canopener at 5mm deflection.
So you turned to hot bending:- heat to cherry red
- let cool down slowly by air (=annealing)
- once it cooled down: bend with hammer
- heat up again to cherry red
- dunk in water (=hardening)
- no tempering
- sharpen
- annihilate can
Is this all correct?
Remarks?
Any idea of temperatures?
Do you think the hardening without tempering has left it too brittle for hard use? -
Looks like Zoidberg did some serious testing on that can in the photos

-
Nicely done zoid !

-
@Rebelgium said:
@Zoidberg wicked! Thanks for the experiments, very interesting!
So let me recap to see if I got this correctly:Cold bending with hammer snapped the canopener at 5mm deflection.
So you turned to hot bending:- heat to cherry red
- let cool down slowly by air (=annealing)
- once it cooled down: bend with hammer
- heat up again to cherry red
- dunk in water (=hardening)
- no tempering
- sharpen
- annihilate can
Is this all correct?
Yes, this is all correct.
@Rebelgium said:
Remarks?Don't bother with cold bending.
@Rebelgium said:
Any idea of temperatures?I think the map fuel flame air temp is around 2000°C.
@Rebelgium said:
Do you think the hardening without tempering has left it too brittle for hard use?Good question. Define hard use. When I can find the time I'll test it to failure.
-
Great work on that, Zoidberg.
I wholeheartedly approve of test-to-failure.


If I were to guess, the lack of annealing will leave it more brittle than it was originally, but I'm not sure harder/more brittle is a bad thing with a can opener. They're not really subject to that much flex in use.
-
Specifications on various alloys usually have some information and specific recipes for annealing and hardening treatments of that particular steel quality. For 420 stainless steel an example can be found at http://www.aksteel.com/pdf/markets_products/stainless/martensitic/420_data_sheet.pdf
Hello! It looks like you're interested in this conversation, but you don't have an account yet.
Getting fed up of having to scroll through the same posts each visit? When you register for an account, you'll always come back to exactly where you were before, and choose to be notified of new replies (either via email, or push notification). You'll also be able to save bookmarks and upvote posts to show your appreciation to other community members.
With your input, this post could be even better 💗